无双酚A通用粘接剂对健康及龋影响牙本质的粘接性能
Bonding Performance of a Bisphenol A-Free Universal Adhesive to Sound and Caries-Affected Dentin.
Bonding Performance of a Bisphenol A-Free Universal Adhesive to Sound and Caries-Affected Dentin.
当前通用型粘接剂对龋影响牙本质的粘接性能不可靠,并会释放双酚A(BPA)。本研究比较了一种无BPA通用型粘接剂与其前代产品(含双酚类)在健康牙本质和龋影响牙本质上的粘接性能及界面特征。本研究使用240颗人磨牙:120颗为健康牙本质,120颗为龋影响牙本质(CAD)。制备牙本质表面后,分别使用Scotchbond Universal Plus(SBUP/无BPA)或Scotchbond Universal(SBU/含BPA),采用酸蚀-冲洗(ER)或自酸蚀(SE)模式进行粘接。树脂-牙本质粘接试件(1 mm²)于水中储存24小时和1年后进行微拉伸粘接强度(μTBS)测试。通过扫描电子显微镜(SEM)分析断裂面图像。数据采用三因素方差分析和Bonferroni事后检验(α < 0.05)。每组另制备3颗牙齿,将粘接剂用荧光染料(罗丹明B)染色,以评估粘接剂向牙本质的扩散情况。纵向切片后,制备的界面储存24小时和1年,浸入荧光素染料中,在共聚焦激光扫描显微镜(CLSM)和SEM下检查(n = 3)。24小时时,CAD在所有组中的μTBS平均值均显著低于健康牙本质(p < 0.0001)。健康牙本质上的SE模式未显示降解或荧光素渗透迹象。ER模式下的SBU(CAD)在两个储存期均显示最低的μTBS平均值。两种粘接剂的ER模式在健康牙本质和CAD的混合层下方随时间推移均显示暴露的胶原纤维和荧光素渗透。尽管SBUP在CAD中显示出更深的粘接剂扩散,但水储存一年后,SBUP(ER和SE)与SBUSE之间的μTBS无显著差异。无BPA和含BPA粘接剂对健康牙本质均产生相似的短期和长期μTBS。对CAD的粘接强度因材料和处理模式而异。SEM图像的定性表现提示,无BPA粘接剂在24小时时可能增强CAD中的界面扩散。然而,两种粘接剂在水储存一年后均表现出降解。
Current universal adhesives exhibit unreliable bonding to caries-affected dentin and release bisphenol A (BPA). This study compares a BPA-free universal adhesive with its predecessor (bisphenol-based) to assess bonding performance and interfacial characteristics on sound and caries-affected dentin. Two hundred forty human molars were used in this study: 120 with sound dentin and 120 with caries-affected dentin (CAD). The dentin surfaces were prepared and bonded with Scotchbond Universal Plus (SBUP/BPA-free) or Scotchbond Universal (SBU/BPA-containing) using etch-and-rinse (ER) or self-etching (SE) modes. Resin-dentin bonded specimens (1 mm2) were stored in water for 24 hours and one year and tested for microtensile bond strength (μTBS). The failure images were analyzed through scanning electron microscopy (SEM). Data were submitted to three-way ANOVA and Bonferroni post hoc tests (α < 0.05). Three additional teeth were prepared for each group for evaluation of adhesive diffusion into dentin by dyeing the adhesives with a fluorochrome (Rhodamine B). After longitudinal sectioning, the generated interfaces were stored for 24 hours and one year, immersed in fluorescein dye and examined under confocal laser scanning microscopy (CLSM) and SEM (n = 3). CAD showed μTBS mean values significantly lower (p < 0.0001) than those of sound dentin for all groups at 24 hours. The SE mode on sound dentin showed no signs of degradation or fluorescein infiltration. SBU in the ER mode (CAD) showed the lowest mean μTBS in both storage periods. The ER mode for both adhesives showed exposed collagen fibrils and fluorescein infiltration underneath the hybrid layer of the sound and CAD over time. Although SBUP showed deeper adhesive diffusion into the CAD, no significant difference in μTBS was found between SBUP (ER and SE) and SBUSE after a year of water storage. Both the BPA-free and BPA-containing adhesives produced similar short- and long-term μTBS to sound dentin. Bond strengths to CAD varied by material and conditioning mode. Qualitative appearance of SEM images suggests that interfacial diffusion in CAD at 24 hours may be enhanced for the BPA-free adhesive. However, both adhesives exhibited degradation after one year of water storage.
C S Garfias, M F De Goes. Bonding Performance of a Bisphenol A-Free Universal Adhesive to Sound and Caries-Affected Dentin.. Operative dentistry. 2026; doi:10.2341/24-170-L.
C S Garfias, M F De Goes (2026). Bonding Performance of a Bisphenol A-Free Universal Adhesive to Sound and Caries-Affected Dentin.. Operative dentistry. https://doi.org/10.2341/24-170-L
C S Garfias, M F De Goes. Bonding Performance of a Bisphenol A-Free Universal Adhesive to Sound and Caries-Affected Dentin.[J]. Operative dentistry, 2026 doi:10.2341/24-170-L.
翻译全文 · AI 文献问答 · PDF 原文下载 · 引用导出