不同表面处理对可流动单层块状填充复合材料修复粘结强度的影响
Effect of different surface treatments on the repair bond strength of flowable single-shade bulk-fill composites.
Effect of different surface treatments on the repair bond strength of flowable single-shade bulk-fill composites.
评估不同表面处理方法对流动型单色大块填充复合树脂修复剪切粘接强度(SBS)的影响。使用纳米混合型复合树脂(GrandioSo,VOCO)制作200个复合树脂圆盘,以模拟老化修复体。所有试件均经过5,000次热循环以模拟口腔老化。测试了五种不同的表面处理方法:不处理(对照组)、金刚砂车针打磨、磷酸酸蚀、Er,Cr:YSGG激光照射和硅烷涂布。处理后,使用通用粘接剂(Tokuyama Universal Bond)将三种流动型单色大块填充复合树脂:Omnichroma Flow Bulk(Tokuyama Dental)、SimpliShade Bulk Fill Flow(Kerr)和Charisma Bulk Flow ONE(Kulzer)粘接于老化表面。使用万能试验机测量SBS,并在体视显微镜下检查失败模式。采用稳健方差分析和卡方检验进行统计分析(α= 0.05)。树脂复合树脂类型、表面处理方案及其交互作用均对SBS值有显著影响(P< 0.001)。在测试组中,GrandioSo联合硅烷处理的SBS最高(23.85 MPa),而Charisma Bulk Flow ONE在酸蚀后的SBS最低(10.8 MPa)。与其他处理相比,硅烷涂布显著提高了SBS(P< 0.001)。粘接失败最常见于酸蚀组和对照组,而激光组和硅烷组则更多表现为内聚失败和混合失败。有效的表面处理对于持久且可预测的复合树脂修复至关重要。硅烷涂布和Er,Cr:YSGG激光照射显著提高了流动型单色大块填充复合树脂的修复粘接强度,而单独磷酸酸蚀则不足。
To assess how various surface treatment methods affect the repair shear bond strength (SBS) of flowable single-shade bulk-fill composite resins. 200 composite discs were fabricated using a nanohybrid composite (GrandioSo, VOCO) to simulate aged restorations. All specimens underwent 5,000 thermal cycles to mimic oral aging. Five different surface treatment approaches were tested: no treatment (control), diamond bur abrasion, phosphoric acid etching, Er,Cr:YSGG laser irradiation, and silane application. After treatment, three flowable single-shade bulk-fill composites: Omnichroma Flow Bulk (Tokuyama Dental), SimpliShade Bulk Fill Flow (Kerr), and Charisma Bulk Flow ONE (Kulzer) were bonded onto the aged surfaces using a universal adhesive (Tokuyama Universal Bond). SBS was measured with a universal testing machine, and failure modes were examined under a stereomicroscope. Statistical analyses were conducted with robust ANOVA and chi-square tests (α= 0.05). Both resin composite type and the surface treatment protocol, as well as their interaction, had significant effects on SBS values (P< 0.001). Among the tested groups, the highest SBS was recorded for GrandioSo combined with silane treatment (23.85 MPa), while the lowest was found for Charisma Bulk Flow ONE after acid etching (10.8 MPa). Silane application resulted in significantly greater SBS compared to other treatments (P< 0.001). Adhesive failures were most prevalent in the acid and control groups, whereas laser and silane groups displayed more cohesive and mixed failures. Effective surface conditioning is essential for durable and predictable composite repairs. Silane application and Er,Cr:YSGG laser irradiation significantly improved the repair bond strength of flowable single-shade bulk-fill composites, whereas phosphoric acid etching alone was insufficient.
Betül Kübra Kurucu Karadeniz, İbrahim Doğan. Effect of different surface treatments on the repair bond strength of flowable single-shade bulk-fill composites.. American journal of dentistry. 2026;
Betül Kübra Kurucu Karadeniz, İbrahim Doğan (2026). Effect of different surface treatments on the repair bond strength of flowable single-shade bulk-fill composites.. American journal of dentistry.
Betül Kübra Kurucu Karadeniz, İbrahim Doğan. Effect of different surface treatments on the repair bond strength of flowable single-shade bulk-fill composites.[J]. American journal of dentistry, 2026
翻译全文 · AI 文献问答 · PDF 原文下载 · 引用导出